X36CrMo17
| Chemical Composition (%) | C | Si | Mn | Cr | Mo | Ni |
| % Average | 0,36 | ≤1,00 | ≤1,50 | 16,00 | 1,10 | ≤1,00 |
| DIN Analysis | 0,33-0,45 | 0,10-1,00 | 0,10-1,50 | 15,50-17,50 | 0,80-1,30 | 0,01-1,00 |
| Thermal Conductivity ( W/ m.K ) | 20°C | 350°C | 700°C |
| 17,2 | 21,0 | 24,7 |
| HEAT TREATMENT | |||
| Tempature(°C) | Time (Hour) | Cooling Environment | |
| Soft Annealing | 780-820 | 2-5* | Furnace |
| Stress Relief Annealing | 600-650 | 2* | Furnace |
| Hardening | 1000-1040 | - | Oil, Hot bath 500-550°C |
| Tempering | 600-680 | 1 hour for every 20 mm | Air |