X36CrMoV5-1
Chemical Composition (%) | C | Si | Mn | Cr | Mo | V |
% Average | 0,36 | 0,50 | 0,30 | 5,00 | 1,35 | 0,45 |
DIN Analysis | 0,32-0,40 | 0,1-0,50 | 0,1-0,50 | 4,60-5,40 | 1,10-1,60 | 0,35-0,60 |
Thermal Conductivity ( W/ m.K ) | 20°C | 350°C | 700°C |
29,8 | 30,0 | 33,4 |
HEAT TREATMENT | |||
Tempature(°C) | Time (Hour) | Cooling Environment | |
Soft Annealing | 750-800 | 2-5* | Furnace |
Stress Relief Annealing | 600-650 | 2* | Furnace |
Hardening | 1010-1040 | - | Air, Oil, Hot bath 500-550°C |
Tempering | 500-650 | 1 hour for every 20 mm saat | Air |