X100CrMoV5-1 / AISI: A2
| Chemical Composition (%) | C | Si | Mn | Cr | Mo | V |
| % Average | 1,00 | 0,25 | 0,60 | 5,30 | 1,05 | 0,25 |
| DIN Analysis | 0,95-1,05 | 0,10-0,40 | 0,40-0,80 | 4,80-5,50 | 0,90-1,20 | 0,15-0,35 |
| Thermal Conductivity ( W/ m.K ) | 20°C | 350°C | 700°C |
| 15,8 | 26,7 | 29,1 |
| HEAT TREATMENT | |||
| Tempature(°C) | Time (Hour) | Cooling Environment | |
| Soft Annealing | 800-840 | 2-5* | Furnace |
| Stress Relief Annealing | 600-650 | 2* | Furnace |
| Hardening | 930-970 | - | Oil, Hot bath 500°C, Air |
| Tempering | 160-540 | 1 hour for every 20 mm | Air |