X210CrW12 / AISI: D6
Chemical Composition (%) | C | Si | Mn | Cr | V |
% Average | 2,10 | 0,25 | 0,45 | 12,00 | 0,70 |
DIN Analysis | 2,00-2,30 | 0,10-0,40 | 0,30-0,60 | 11,00-13,00 | 0,60-0,80 |
Thermal Conductivity ( W/ m.K ) | 20°C | 350°C | 700°C |
16,7 | 20,5 | 24,2 |
HEAT TREATMENT | |||
Tempature(°C) | Time (Hour) | Cooling Environment | |
Soft Annealing | 800-840 | 2-5* | Furnace |
Stress Relief Annealing | 600-650 | 2* | Furnace |
Hardening | 950-980 | - | Oil, Hot bath 500-550°C, Air |
Tempering | 150-300 | 1 hour for every 20 mm | Air |